CRU-WEAR的热处理工艺?
请问有哪位高手知道CRU-WEAR的热处理工艺的,请指教一下!小弟不甚感谢。属于模具钢 Hardening Data
Air cooled from austenitizing temperature shown and double tempered 2+2 hours.
Tempering HEAT TREAT RESPONSE
Temperature 1850F 1950F2050F
°F °C (1010C)(1065C)(1120C)
AQ 63-65 63-65 62-64
900 480 61-63 62-64 61-63
950 510 61-63 62-64 64-66
1000 540 57-59 60-62 63-65
1025 550 56-58 58-60 61-63
1050 565 54-56 55-57 59-61
不知道这个数据够详细吗