zjy95381 发表于 2010-4-19 20:27:05

请问高鉻铸铁的脱稳处理是怎么回事?

怎么个处理法?是不是脱稳处理完了后,再将铸件重新加热到淬火温度再淬火啊?还是淬火之前的保温就叫脱稳处理啊?请教,谢谢

qjohn 发表于 2010-6-18 14:56:47

本帖最后由 qjohn 于 2010-6-18 15:04 编辑

查了一下文献,大概是这样说的。希望对你有帮助。

Destabilisation heat treatment

1.The destabilisation (or conditioning) heat treatment involves holding at a temperature between 920 and 1060 for 1-6 h. At this temperature, secondary carbides precipitate in the matrix, reducing the matrix alloy content, and in particular, the carbon content. The reduced alloy content of the austenitic matrix increases the M; temperature, so that on cooling to room temperature, the matrix may transform to martensite. Air cooling from the destabilisation temperature is usually sufficient to produce a predominantly martensitic structure while avoiding quench cracking, though lower chromium alloys may be oil quenched.

2.The destabilization heat treatmen: involves holding at temperatures of around I000°C to precipitate secondary carbides in the austenite, thereby reducing the alloy content of the matrix. This destabilized austenite more readily transforms to martensite upon cooling to room temperature.
页: [1]
查看完整版本: 请问高鉻铸铁的脱稳处理是怎么回事?