mho88 发表于 2011-3-14 11:58:12

网带炉怎么检测漏气

请教各位:网带炉怎么检测漏气?我们公司用的苏州胜龙的网带炉,出来的产品边缘发黑,想验证是不是炉子漏气,不知道有什么方法?

197971500 发表于 2011-3-24 09:03:03

做网带炉的高手们来讲一下啊。

xhyy2008 发表于 2011-3-24 09:40:16

工程师开腔呀,怎么没人响应

stingrui 发表于 2011-3-24 13:57:57

可以看看气氛,CO2含量是不是串高

wic 发表于 2011-3-25 09:35:51

轉自http://asm.informz.net/ASM/archives/archive_1379002.html

Q: Can I determine where the oxidation on my heat treated parts is coming from within my furnace?

A: When checking a continuous furnace, oxidation in the preheat section has a matte or frosted appearance and is usually caused by air infiltration from the entrance of the furnace. Hot zone oxidation may cause scaly or blistered parts. This generally occurs from elevated moisture or oxygen levels due to improper atmosphere balance or water/air leaks in the cooling zone. Cooling zone oxidation typically results in a smooth, sometimes shiny discoloration—poor curtain design, excessive belt speed, water leaks, or insufficient atmosphere flow rates are possible causes.

In batch furnaces, start by identifying the oxidant causing the problem. Flowing nitrogen and measuring the oxygen and moisture levels can give an indication of the oxidant involved. Then, a review of typical leak sources, such as seals, fittings, unions, and weld joints usually leads to discovery of the leak source.

Answered by Mark Lanham, Air Products Applications Engineer

zHANG_999567 发表于 2011-3-25 10:41:50

如果炉子漏气应该是局部,也就是说产品发黑数量不是很多,而且是整体发黑的.