[Discussion] Major difference for AMS 2750 E & F

[复制链接]

签到天数: 96 天

[LV.6]常住居民II

发表于 2020-8-7 14:04:58 | 显示全部楼层 |阅读模式
北京中仪天信科技有限公司
Let's discuss the big change for AMS 2750 E & F

1. Periodic TUS requirements
    For E version the max. and min. temperature TUS is required once per calendar year but for version F, it is reuqired annually.

2. For concinous furnace periodic TUS
    For E version, no max. and min. transvers spped requirement, periodc TUS can be performed at any traverse speed is ok but for Version F A TUS shall be performed at the highest and lowest traverse speeds used during production at least annually.

Generally for TUS test, the requirements is more strict.

Any other big change?

Appreciated your sharing and discussion.

评分

参与人数 1热处理币 +40 收起 理由
cjzhou + 40 感谢参与!

查看全部评分

签到天数: 8 天

[LV.3]偶尔看看II

发表于 2021-2-8 16:13:59 | 显示全部楼层
how to say  I think SAT is key point ,TUS if use N type thermocouple , it is not accurate ,
and who to make  ranking method for furnace  

评分

参与人数 1热处理币 +20 收起 理由
cjzhou + 20 感谢参与!

查看全部评分

回复 顶 踩

使用道具 举报

签到天数: 96 天

[LV.6]常住居民II

 楼主| 发表于 2021-3-1 14:46:03 | 显示全部楼层
sswpyq594596 发表于 2021-2-8 16:13
how to say  I think SAT is key point ,TUS if use N type thermocouple , it is not accurate ,
and wh ...

Thanks for sharing your pinion.

We don't use Type N sensors but only J.

But I agree with you.

There is a big change for Alternate SAT, especially for the documentation requirements of  Alternate SAT result.

It seems much more records are needed to comply with the F version requirements.

Do you also have the Alternate SAT in your company?
回复 顶 踩

使用道具 举报

签到天数: 96 天

[LV.6]常住居民II

 楼主| 发表于 2021-3-1 14:53:42 | 显示全部楼层
Some other changes for the TUS requirements:

3.5.14.1.3
The time required to achieve TUS sensor temperature recovery, stabilization or a recurrent temperature pattern shall not have exceeded the time limit specified in the applicable material or process specification.
---Usually the technical documents only have the requriements for Soaking phase but no requirements for the time achived temperature recorvery?
What's your opinion for this new requirements?

评分

参与人数 1热处理币 +20 收起 理由
cjzhou + 20 感谢支持!

查看全部评分

回复 顶 踩

使用道具 举报

签到天数: 96 天

[LV.6]常住居民II

 楼主| 发表于 2021-4-1 13:30:53 | 显示全部楼层
3.5.14 TUS Pass/Fail Requirements
3.5.14.1.4 The TUS soak period shall not have been less than the minimum required time.

For this new requirement about the soak period, can we explicited the requirement that the TUS soaking start time shall be at least equile or earlier than the Hea treatment equipment soaking start time?

Appriciated very much for your opinion in advance.

评分

参与人数 1热处理币 +20 收起 理由
cjzhou + 20 感谢参与!

查看全部评分

回复 顶 踩

使用道具 举报

签到天数: 96 天

[LV.6]常住居民II

 楼主| 发表于 2021-7-13 14:43:59 | 显示全部楼层
One big change for us is that the over-temperature instrument calibration is also needed according to AMS 2750F.

Previously we didn't perform the calibration for over-temperature instrument. Now we have to do some improvement for this.

评分

参与人数 1热处理币 +20 收起 理由
cjzhou + 20 感谢参与!

查看全部评分

回复 顶 踩

使用道具 举报

签到天数: 124 天

[LV.7]常住居民III

发表于 2021-11-2 13:30:21 | 显示全部楼层
one big change for TUS data collection F 3.5.10:
. is If the furnace or refrigeration equipment is pre-stabilized, data collection shall begin prior to the TUS sensors being inserted.
  Was If the furnace is prestabilized, data collection shall begin as soon as the test load or rack is loaded in the furnace.
回复 顶 踩

使用道具 举报

您需要登录后才可以回帖 登录 | 立即注册

本版积分规则

QQ|Archiver|手机版|小黑屋|热处理论坛 ( 苏ICP备2021037530号|苏公网安备32059002001695号 )