[Help] Heat up factor for Alluminum alloy solution heat treatment in Continuous furnace

[复制链接]

签到天数: 96 天

[LV.6]常住居民II

发表于 2018-4-26 08:51:24 | 显示全部楼层 |阅读模式
北京中仪天信科技有限公司
Dears

       Would you please kindly share how to define the heat up factor for Aluminum which is solution heat treated in continuous furnace?

Is there any relationship between the heat up factor and the furnace speed?

Thanks very much for sharing.

评分

参与人数 1热处理币 +16 收起 理由
cjzhou + 16 感谢参与!

查看全部评分

签到天数: 96 天

[LV.6]常住居民II

 楼主| 发表于 2018-4-27 08:22:35 | 显示全部楼层
Who can share any information for the heating up factor or how to define the total time in the continuous furnace when performing the solution heat treatment?

Thanks very much.
回复 顶 踩

使用道具 举报

签到天数: 993 天

[LV.10]以坛为家III

发表于 2018-4-28 22:08:27 | 显示全部楼层
u Englishgood good。           
回复 顶 踩

使用道具 举报

签到天数: 96 天

[LV.6]常住居民II

 楼主| 发表于 2018-5-4 13:29:55 | 显示全部楼层



But there isn't any feedback about this question.

Maybe I didn't make myself understood.

I think it should be right that the faster the furnace speed is, the greater the heat up factor is.

Thanks all.
回复 顶 踩

使用道具 举报

签到天数: 299 天

[LV.8]以坛为家I

发表于 2018-5-19 09:59:26 | 显示全部楼层
Would you like to introduce somethingmore  about the heat up factor?

评分

参与人数 1热处理币 +5 收起 理由
cjzhou + 5 感谢参与!

查看全部评分

回复 顶 踩

使用道具 举报

签到天数: 224 天

[LV.7]常住居民III

发表于 2018-5-28 14:34:53 | 显示全部楼层
Well, I'm not sure what is the heat up factor. ;

评分

参与人数 1热处理币 +5 收起 理由
cjzhou + 5 感谢参与!

查看全部评分

回复 顶 踩

使用道具 举报

签到天数: 171 天

[LV.7]常住居民III

发表于 2018-7-14 15:26:05 | 显示全部楼层
Is it the heating up speed?

评分

参与人数 1热处理币 +5 收起 理由
cjzhou + 5 感谢参与!

查看全部评分

回复 顶 踩

使用道具 举报

签到天数: 96 天

[LV.6]常住居民II

 楼主| 发表于 2018-10-11 13:30:23 | 显示全部楼层
我心飞翔eric 发表于 2018-5-19 09:59
Would you like to introduce somethingmore  about the heat up factor?

We define the heat up dactor as: heating up time / plate thickness

(Heating up time means the time needed to reaching soaking time from the plate entring the continous furnace)

Thanks!
回复 顶 踩

使用道具 举报

签到天数: 96 天

[LV.6]常住居民II

 楼主| 发表于 2018-10-11 13:31:46 | 显示全部楼层
我心飞翔eric 发表于 2018-5-19 09:59
Would you like to introduce somethingmore  about the heat up factor?

We define the heat up dactor as: heating up factor= heating up time / plate thickness

(Heating up time means the time needed to reaching soaking time from the plate entring the continous furnace)

Thanks!
回复 顶 踩

使用道具 举报

签到天数: 96 天

[LV.6]常住居民II

 楼主| 发表于 2018-10-11 13:32:31 | 显示全部楼层
leekeychen 发表于 2018-7-14 15:26
Is it the heating up speed?

It seems the heating up factor is not a commen defination.

We define the heat up dactor as: heating up factor= heating up time / plate thickness

(Heating up time means the time needed to reaching soaking time from the plate entring the continous furnace)

Thanks!
回复 顶 踩

使用道具 举报

签到天数: 96 天

[LV.6]常住居民II

 楼主| 发表于 2018-10-11 13:33:15 | 显示全部楼层
lydia 发表于 2018-5-28 14:34
Well, I'm not sure what is the heat up factor. ;

It's my fualt.

I forgot the heating up factor was not a commen defination for HT.

We define the heat up dactor as: heating up factor= heating up time / plate thickness

(Heating up time means the time needed to reaching soaking time from the plate entring the continous furnace)

Thanks!

评分

参与人数 1热处理币 +5 收起 理由
cjzhou + 5 感谢参与!

查看全部评分

回复 顶 踩

使用道具 举报

签到天数: 27 天

[LV.4]偶尔看看III

发表于 2018-10-17 14:31:16 | 显示全部楼层
You shall define 'heat up factor' in your procedure.
As I know, it is not always called this name.

Then some tests are needed for the defination of heat up factor.
Of course, the different thickness and load shall also be considered.
I think you can select or define several load situations, and gather applicable heat up factors. Then define the different factors summarised through the tests.
And the operators can follow the work instrustructions.
回复 顶 踩

使用道具 举报

签到天数: 96 天

[LV.6]常住居民II

 楼主| 发表于 2021-4-14 16:14:01 | 显示全部楼层
hackyue 发表于 2018-10-17 14:31
You shall define 'heat up factor' in your procedure.
As I know, it is not always called this name.
...

Thanks so much.

Now we defined the new heat up factor based on several tests.
回复 顶 踩

使用道具 举报

签到天数: 27 天

[LV.4]偶尔看看III

发表于 2021-4-14 21:34:56 | 显示全部楼层
LucySun 发表于 2021-4-14 16:14
Thanks so much.

Now we defined the new heat up factor based on several tests.

Glad to hear it works.
回复 顶 踩

使用道具 举报

您需要登录后才可以回帖 登录 | 立即注册

本版积分规则

QQ|Archiver|手机版|小黑屋|热处理论坛 ( 苏ICP备2021037530号|苏公网安备32059002001695号 )
Copyright © 2005-2026, rclbbs.com 苏州热协网络技术有限公司 版权所有

GMT+8, 2026-11-25 09:10 , Processed in 0.027941 second(s), 22 queries .

Powered by Discuz! X3.5

© 2001-2026 Discuz! Team.

快速回复 返回顶部 返回列表