in our company,bear rings after heat traetmented,they will become larger.
we use atmosphere protected continues net furnance,
use  propane(丙烷) carbinol(甲醇) nitrogen(氮气)as protected atmosphere.
bear outer rings' demensions at the range of 30mm to 130mm,after treated, the average largeness is 0.25%D.
is it nomarl?will it infulence the quanlity and serverce life?

签到天数: 7 天

[LV.3]偶尔看看II

发表于 2009-4-9 10:07:28 | 显示全部楼层
ja, Distortion is unavoidable.
After heattreatment, the dimension usually change.

But this change or vary, also has regular patern.

So we need to follow these distortion regular(law).

The attachment file give  experience for gear ring.

大型渗碳齿轮圈热处理畸变与控制.pdf

308.81 KB, 下载次数: 48

回复 顶 踩

使用道具 举报

该用户从未签到

发表于 2009-4-9 10:15:27 | 显示全部楼层
Yes, distortion is a difficulty problem for heattreatment.

Although vacuum heattreatment could not avoid this problem!

less dietortion, less oxidation, are the purpose of heat treatment industry!
回复 顶 踩

使用道具 举报

该用户从未签到

发表于 2009-4-9 15:11:02 | 显示全部楼层
The diameter of the ring-like work-piece heat–treated become larger,I think it is the normal phenomenon. you may reserve grinding allowance to solve.
回复 顶 踩

使用道具 举报

签到天数: 2 天

[LV.1]初来乍到

发表于 2009-4-11 18:23:21 | 显示全部楼层
it's normal for the products that have cylinder shape go 'bigger'
you can collect this distortion date for the mass production, then, make allwance for the machining process.
回复 顶 踩

使用道具 举报

您需要登录后才可以回帖 登录 | 立即注册

本版积分规则

QQ|Archiver|手机版|小黑屋|热处理论坛 ( 苏ICP备2021037530号|苏公网安备32059002001695号 )
Copyright © 2005-2026, rclbbs.com 苏州热协网络技术有限公司 版权所有

GMT+8, 2026-11-25 09:39 , Processed in 0.025021 second(s), 24 queries .

Powered by Discuz! X3.5

© 2001-2026 Discuz! Team.

快速回复 返回顶部 返回列表