本帖最后由 所以因为 于 2013-4-22 11:06 编辑
leomet 发表于 2008-3-3 08:34 static/image/common/back.gif
我中文打字很慢, 僅分享我典藏的相片. 並不想討論.
如果有人帮忙解释给新手学习学习, 我不反對. 有不足处 ...
Hello WU Lao! I would like to introduce these beauties (Microstructure picture) to these old or young Heat Treatment Men. I will do the job by the way of expressing my understanding about these pictures and ask some questions and you can give your comments.
Question 1: Why does the carbide precipitate inside the high temperature ferrite but not inside the austenite in stainless steel as cast condition (Fig.固溶前.jpg)? Cr% does the job? I ever detected decarbonization of a fusion line of a weld joint with different base material. The two kinds of base material have different Cr% equivalence. This phenomenon is called "carbon removal". is there other explanation from you ?
Highest esteem !!!!!
After solution treatment, the carbon goes into the austenite and Delta ferrite (= high temperature ferrite) lattices as the C atom. So no carbide reveals any more.I think the C% is the same between austenite and ferrite because there is no diffusion. The delta ferrite is in rich of Cr% equivalence, it will transfer to be a new substance under some conditions, that is a bad thing.
Professor Wu.,have you ever catch some metallographs about cemented carbide or others P.M
本帖最后由 leomet 于 2013-5-9 20:52 编辑
AISI 52100 國際大廠軸承 測試運轉幾小時後就生噪音 (不良率: 1~2/100).
硬度: HRC 59~60
晶间碳化物太多了,机加工前正火没正好
sbfcbj 发表于 2013-4-22 22:03 static/image/common/back.gif
晶间碳化物太多了,机加工前正火没正好
碳化物分布还算均匀,感觉好像有非马氏体组织。望吴老给予最终解答。
leomet 发表于 2008-3-8 05:39 static/image/common/back.gif
45钢 溼式 离合器片 5, 6年前有人要我開發此產品 當年剖析的
摩擦材料/基板 界面
这是一种自润滑复合材料
这位才是热处理论坛中的高手,当之无愧的应当称老师。感谢您提供的照片,解决了我很多困惑。
楼主的制样水平真是让人佩服啊!收益匪浅!
leomet 发表于 2008-3-3 08:34 static/image/common/back.gif
我中文打字很慢, 僅分享我典藏的相片. 並不想討論.
如果有人帮忙解释给新手学习学习, 我不反對. 有不足处 ...
你好,请问不锈钢腐蚀后为什么会出现腐蚀坑,怎么造成的?
leomet 发表于 2008-3-9 17:34 static/image/common/back.gif
QT的金相 ductile iron, carbide is tinted pink. pearlite,green to blue.
[ 本帖最后由 leomet 于 2 ...
so beautiful吴老师辛苦了,感谢吴老师!
:L都是天才+人才啊,神马时候我也能露个脸让大家羡慕、嫉妒、恨啊
很好的东西,收藏了,谢谢分享~:)
leomet 发表于 2008-3-21 11:37 static/image/common/back.gif
过共晶成份
[ 本帖最后由 leomet 于 2008-8-16 10:27 编辑 ]
请问初晶和共晶怎么区分啊!!!谢谢!!!
yuyu1010 发表于 2008-7-27 11:16 static/image/common/back.gif
出现了脱碳现象貌似!!
其实碳原子发生了扩散.
leomet 发表于 2008-3-1 12:23 static/image/common/back.gif
前述氮化钢 tie bar, 以火焰切割取试片. 试片自高温冷却, 在不同温度范围相变化所得组织. 未经color etchin ...
很典型的图片,感谢分享。
应该是大颗粒碳化物多了。还有分布也不均。
吴老师非常感谢您将多年的积累上传,供我们后辈学习。您的金相图片非常的棒,
前几天领导还说要我多看看金相图片,非常感谢您的分享,先收藏起来,慢慢消化。
leomet 发表于 2008-11-15 16:17 static/image/common/back.gif
砂輪切割熱 引起的相變化
一塊(前三張)昇溫較高, 生高碳M+殘奧; 晶界微熔後急冷生碳化物.
前辈您好!请问后面几张图片黑色针状组织周边的白色组织是什么呢?如何形成的?谢谢!
本帖最后由 leomet 于 2014-6-2 15:35 编辑
P/M high speed steel, tempered and most of the R.A. in the matrix is gone.